Indentation: Basic usage
Introduction
The toolbox aims to help with nanoindentation data analysis using python.
Note
The following units should be used: [mN], [µm], [GPa] because the area function is unit-dependent.
Calculations are carried out by the default Oliver-Pharr Method.
Data in indentation experiment includes Method, Vendor, Indenter tip
Method: ISO, CSM
Vendor: Agilent, Hysitron, FischerScope, Micromaterials
Indenter Tip: shape of indenter tip and stiffness of gantry
How it works:
Obtain loading and unloading data through nanoindentation, measuring force (p) and depth (h)
Calculate:
slope [mN/µm]: Slope of unloading part (stiffness)
hc [µm]: Contact depth
Ac [µm2]: Contact area
hardness [GPa]
modulusRed [GPa]: reduced Young’s modulus
modulus [GPa]: Young’s modulus
Plot
Initialization
Import necessary libraries:
import matplotlib.pyplot as plt
import numpy as np
from nanoindentation import Indentation, Tip
Introduce tip:
ourTip = Tip() #µm/mN
Initialization: Files containing the experimental data are in hdf5, txt or xls format:
fileName = 'Nafion_15_100_5.hdf5'
Introduce class Indentation, where nuMat is material’s Poisson’s ratio:
i = Indentation(fileName, nuMat=0.3, tip=ourTip)
Run through all indentations (Test 1, Test 2, etc) in the file with a for cycle:
for testname in i:
<body>
In the <body> one can analyse the data and create the plots to be viewed like following:
Calculate all the relevent data from the indent: stiffness S [mN/µm], maximum depth hMax [µm], maximum force pMax [mN], reduced Young’s modulus redE [GPa], contact area A [µm2], contact depth hc [µm], Young’s modulus E [GPa], hardness H [GPa]:
i.analyse()
Plotting:
i.plotwould plot each test(indent) independantly with the analysis data: slope, hc, power law etcplt.plot(i.h, i.p)would plot all tests(indents) together. Useful to spot outliers:i.plot() plt.plot(i.h, i.p)
Save all values to a dictionary. This can be appended to a user defined dataframe and further information can be added to it accordingly. E.g. the file name in this case:
meta = i.metaUser
meta["file name"]=fileName
df = df.append(meta, ignore_index=True)
Show plots:
plt.show()
Full source code of example
This is an example code analysing the hdf5 files from FischerScope nanoindenter:
import matplotlib.pyplot as plt
import pandas as pd
from nanoindentation import Indentation, Tip
fileName = "Nafion_15_100_5.hdf5"
ourTip = Tip() #um/mN
i = Indentation(fileName, nuMat=0.5, tip=ourTip)
df = pd.DataFrame()
for testname in i:
i.analyse()
#i.plot()
plt.plot(i.h, i.p)
meta = i.metaUser
df = df.append(meta, ignore_index=True)
print(df)
plt.show()